Alloy R41 | ||||||||||||
Chemical composition | ||||||||||||
C | Cr | Ni | Co | Mo | Al | Ti | B | Zr | S | P | Mn | Si |
0.06-0.12 | 18.0-20.0 | Remainder | 10.0-12.0 | 9.0-10.5 | 1.40-1.80 | 3.0-3.5 | ≤5.0 | 0.003-0.010 | ≤0.07≤0.0150 | ≤0.015 | ≤0.5 | ≤0.50 |
Mecanical Performance | |||||
Specification | θ/℃ | Σb/MPa | σ0.2/MPa | δ5% | ψ/% |
Fastener | 20 | ≥1070 | - | ≥8 | ≥10 |
760 | ≥870 |
| ≥8 | ≥10 | |
Bar | 20 | ≥1175 | ≥880 | ≥12 | ≥12 |
800 | ≥735 | ≥635 | ≥15 | ≥20 | |
Plate/strip | 20 | ≤1170 | ≥690 | ≤30 |
|
Circle/cake forging | 20 | ≥835 | ≥620 | ≥12 | ≥15 |
Physical Performance | |||
Melting point | Density | Hardness | Magnetism |
1316-1371℃ | 8.27g/cm3 | ≤363(HBS) | <1.002 H/m |
Alloy R41 Shaping Property:
The steel ingot should be homogenized before forging and the heating temperature is 1100~1180℃.
Alloy R41 Part Heat Treatment Process:
At lower temperature, the parts are required to have high tensile strength and fatigue performance, 1080℃ and air cooling+760℃, 16H, air cooling.
When working at high temperature, it is required that the material has high thermal intensity, and the heat treatment specification is 1180℃ air cooling +900℃ 4H, air cooling.
Alloy R41 Welding Technology:
The alloy can be welded by welding, diffusion welding and friction welding.
Spot delivery, including delivering small batches of goods
Provide wide-range and complete materials series products
Cutting plates, including complex shapes of materials and special processing and disposal
Cutting bars and strips
Our application technology expert provide the best material and recommendation
One-stop service